Magnetic particle and dye penetrant testing
In one sentence: both methods make a crack you can barely see visible: magnetic particles gather where a crack disturbs a magnetic field, and penetrant dye bleeds out of a crack onto a white developer.
Magnetic particle testing (MT)
- Clean the surface (coatings thicker than a little reduce sensitivity).
- Magnetize the area with a yoke (an electromagnet with two legs) placed across the expected crack direction.
- Apply fine iron particles, dry powder or a liquid suspension, often visible or fluorescent.
- Particles gather at leakage fields where a crack interrupts the magnetic flux, showing its line.
- Repeat with the yoke turned about 90 degrees: MT finds cracks best when they run across the field.
Works on ferromagnetic steel only, finds surface and slightly subsurface cracks. Standardized in ASTM E709 and E1444.
Dye penetrant testing (PT)
- Clean and dry the surface thoroughly.
- Apply a red or fluorescent penetrant and wait the dwell time (often 5 to 30 minutes).
- Remove the excess from the surface.
- Apply a thin white developer; penetrant trapped in cracks bleeds out and shows as red lines or glows under UV light.
Works on any non-porous material (steel, stainless, aluminum, welds), finds only surface-breaking defects. Standardized in ASTM E165.
Uses on structures
- Confirming and measuring suspected fatigue cracks at welded details. See Steel defects: corrosion, fatigue cracks and connections.
- Checking weld toes and repairs.
- Inspecting after a crack has been arrested with drilled holes, to see whether the crack tip was caught.
Limits
Both need clean surfaces and good access. Neither tells you how deep a crack goes: use Ultrasonic testing of steel and welds for that.
Common mistakes
- Testing through paint and declaring no cracks.
- Using one yoke orientation only.
- Cutting the penetrant dwell time short.